dc.description.abstract | RESUMEN
En la presente investigación se buscó demostrar la comparación de la resistencia a
compresión axial de un concreto anti-deslave con un concreto normal, los cuales se
realizaron con los mismos diseños de mezcla, se utilizó un aditivo anti-deslave y un
cemento Portlant tipo I, para un concreto de resistencia mínima de 210 kg/cm
2
. Se
inició realizando los ensayos físicos y mecánicos de los agregados que se obtuvieron
de la cantera “La Victoria” de la ciudad de Cajamarca, para posteriormente realizar
el diseño de mezcla. Para obtener un concreto anti-deslave se incorporó al diseño un
porcentaje de aditivo con respecto a la cantidad de cemento en este caso se realizó
con diferentes porcentajes los cuales fueron: 8%, 10% y 12% del peso del cemento,
posteriormente se procedió a la elaboración de los especímenes cilíndricos de
aproximadamente 15 cm de diámetro y 30 cm de altura, estos fueron vaciados bajo
el agua, luego tuvimos que desencofrar y colocar a curar los especímenes el tiempo
establecido para después ser sometidos a ensayos de compresión a los 7, 14 y 28
días y así poder determinar las diferencias en las resistencias a compresión axial de
un concreto anti-deslave con un concreto normal, obteniéndose como resultados que
con los porcentajes del aditivo en relación al peso del cemento y en todas las edades
la resistencia a compresión axial disminuye, lográndose evidenciar la menor pérdida
de resistencia con el porcentaje del 10% del peso del cemento, dándonos un 2.23%
menos que la resistencia de los especímenes patrón, con lo cual no se demuestra la
hipótesis. | es_PE |
dc.description.abstract | ABSTRACT
In this thesis we tried to demonstrate the comparison of the resistance to axial compression
of an anti-washout concrete with a normal concrete, which were made with the same mix
designs, an anti-washout additive and a type I Portlant cement were used. , for a concrete
of minimum resistance of 210 kg / cm
2
. The physical and mechanical tests of the aggregates
that were obtained from the "La Victoria" quarry in the city of Cajamarca were started, and
thus the mix design could be carried out, then to obtain an anti-washout concrete, a
percentage was added to the design. of additive with respect to the amount of cement in
this case was made with different percentages which were: 8%, 10% and 12% of the weight
of the cement, later we proceeded to the elaboration of the cylindrical specimens of
approximately 15 cm in diameter and 30 cm in height. These were emptied underwater,
then we had to dismantle and place to cure the specimens the time established for later to
be subjected to compression tests at 7, 14 and 28 days and thus be able to determine the
differences in the axial compression resistances of a concrete anti-washout with a normal
concrete, obtaining as a result that with the percentages of the additive in relation to the
weight of the cement and in all the ages the resistance to axial compression decreases,
being able to demonstrate the lowest loss of resistance with the percentage of 10% of the
cement weight, giving us 2.23% less than the resistance of the standard specimens, which
does not prove the hypothesis. | es_PE |
dc.description.uri | Tesis | es_PE |
dc.format | application/pdf | es_PE |
dc.language.iso | spa | es_PE |
dc.publisher | Universidad Privada del Norte | es_PE |
dc.rights | info:eu-repo/semantics/openAccess | es_PE |
dc.source | Universidad Privada del Norte | es_PE |
dc.source | Repositorio Institucional - UPN | es_PE |
dc.subject | Resistencia a la compresión | es_PE |
dc.subject | Concreto | es_PE |
dc.subject | Concreto armado | es_PE |
dc.title | Resistencia a compresión axial de un concreto F´C = 210 kg/cm2 con la incorporación de aditivo anti - deslave | es_PE |
dc.type | info:eu-repo/semantics/bachelorThesis | es_PE |
thesis.degree.grantor | Universidad Privada del Norte. Facultad de Ingeniería | es_PE |
thesis.degree.level | Título Profesional | es_PE |
thesis.degree.discipline | Ingeniería Civil | es_PE |
thesis.degree.name | Ingeniero Civil | es_PE |
dc.publisher.country | PE | es_PE |
dc.subject.ocde | https://purl.org/pe-repo/ocde/ford#2.01.01 | es_PE |
thesis.degree.program | Pregrado | es_PE |
dc.description.sede | Cajamarca | es_PE |
renati.discipline | 732016 | es_PE |
renati.level | https://purl.org/pe-repo/renati/level#tituloProfesional | es_PE |
renati.type | https://purl.org/pe-repo/renati/type#tesis | es_PE |